Answer first. EN 660-2 is a laboratory test method, not a certificate. It measures how much material a PVC wear layer loses under the Frick-Taber abrasion test, then places the product in one of four wear groups: T (best), P, M, F. The wear group tells you how abrasion-resistant the wear layer is. It does not tell you how much traffic a floor is designed for — that is the use class (EN ISO 10874) — and it says nothing about slip resistance (DIN EN 16165). This guide gives you the group definitions, the report fields worth verifying, and a five-point checklist for choosing a wear class you can defend in a specification.
What EN 660-2 Actually Measures
EN 660-2 — Resilient floor coverings. Determination of wear resistance. Part 2: Frick-Taber test — is a test method standard. It describes how a laboratory measures wear resistance of the wear layer on smooth PVC floor coverings. It is not a product specification standard, not an approval scheme, and it issues no certificate: what it produces is a classification.
Its scope states the purpose precisely — it is intended "particularly for ranking different wear layer types within one type of product." That phrase settles two arguments that recur in tender documents. The ranking is comparative, not absolute: the result orders wear layers against each other inside one product type. And cross-type comparison is not valid: a Group T result on one construction and a Group T result on a different construction are not measured against the same baseline.
So when a datasheet says "EN 660-2 Group T", the verifiable questions are which product type, which sample, which laboratory, and which reported value — a group letter on its own is a statement, while a report with a sample reference and a value is evidence.
The F/M/P/T Scale: What Each Group Means
EN 660-2 results are expressed as volume loss — Fv, in mm³ per 100 cycles — and grouped into four classes. Group T represents the lowest volume loss and therefore the highest abrasion resistance.
| Wear group | Relative ranking | Typical positioning |
|---|---|---|
| Group T | Highest abrasion resistance | Heavy commercial and high-traffic specifications |
| Group P | Second | General commercial areas |
| Group M | Third | Lighter commercial and domestic areas |
| Group F | Lowest abrasion resistance | Light-duty and cushioned products |
Table 1 — EN 660-2 wear groups.
Fv is a volume loss derived from the average mass loss divided by the density of the wear layer, which is why the unit is mm³ rather than milligrams. The group ranks the wear layer; it does not predict service life, because two floors in the same group can still differ once substrate, adhesive, installation and cleaning regime are in play.
| EN 660-2 is… | EN 660-2 is not… |
|---|---|
| a test method for wear-layer abrasion | a product specification standard (those are EN ISO 10581, EN ISO 10582 and EN ISO 11638) |
| reported as a volume loss value plus a group letter | a certificate or an approval |
| valid for ranking wear layers within one product type | a basis for comparing different product types |
| one dimension of durability | a measure of traffic intensity (EN ISO 10874) or slip resistance (DIN EN 16165) |
Table 2 — What EN 660-2 is, and what it is not.
Together the two tables give you the sentence to put in a specification — "wear group per EN 660-2" — and the sentence that keeps you out of trouble: name the standard that actually governs the property you are buying.
How to Read a Wear Test Report
A wear group is only as good as the report behind it. Check six fields before you accept the number:
- Testing laboratory and accreditation — which laboratory issued the report, and under what accreditation.
- Standard and edition — the report should cite EN 660-2, not a vague reference to "abrasion testing".
- Sample identification — product name, thickness, colour or batch. If the sample does not match what you are buying, the result does not transfer.
- Test conditions and method — confirmation that the Frick-Taber method was used.
- Reported result — the volume loss value and the resulting wear group, stated together.
- Report number and date — so the document can be traced and verified.
A group letter printed without a tested value or a named laboratory cannot be verified independently. The fastest way to disqualify a weak offer is to ask for the value and the sample reference.
EN 660-2 vs EN ISO 10874: Two Different Questions
These two standards are constantly quoted as if they were interchangeable. They answer different questions.
| Question | Standard | Example classification |
|---|---|---|
| How abrasion-resistant is the wear layer? | EN 660-2 | Wear group T / P / M / F |
| How much traffic is the floor intended for? | EN ISO 10874 | Class 21–23 domestic, 31–34 commercial, 41–43 light industrial |
Table 3 — Wear group and use class answer different questions.
Neither substitutes for the other. A product can carry a high wear group and still be specified for lighter use; a product with a lower wear group can be classified for areas where abrasion is not the governing factor. A defensible specification states both, for example: wear group T per EN 660-2 (abrasion test report on request); use class 34 per EN ISO 10874. If a tender quotes only one of the two, you cannot tell whether the requirement you are pricing is covered — and neither can the contractor who inherits the risk.
Slip Resistance Is a Separate Standard
Abrasion resistance and slip resistance are different properties, measured by different methods. Slip resistance for commercial flooring is tested under DIN EN 16165 (which replaced DIN 51130) and reported as R classes, typically R9 to R11 indoors. EN 660-2 does not measure slip at all. A floor can be Group T and still be R9; it can be R11 and Group P.
Answering a slip question with a wear group — or the reverse — is the most common specification error in this area, and it usually surfaces after installation, when correcting it is expensive. Specify the two separately:
- Slip: DIN EN 16165 R10, or the rating your project standard requires
- Wear: wear group per EN 660-2
Choosing the Right Class for Your Project
In short: match the wear group to the traffic, the cleaning regime and the replacement cycle — then confirm it against the report rather than the brochure. Use class first, wear group second, verification third; the five criteria below expand that rule.
Criterion 1 — Traffic intensity and type
Start with the use class the area falls into (EN ISO 10874), then look at what actually moves across the floor — pedestrians only, or trolleys, beds and pallet trucks. Sliding and point loads stress a floor differently from foot traffic.
If the area is heavy commercial circulation — hospital corridors, school hallways, transport terminals — then the abrasion requirement sits at the top of the scale. If abrasion is not the governing factor, over-specifying raises cost without changing service life.
Criterion 2 — Cleaning and chemical regime
Frequency and aggressiveness of cleaning matter as much as footfall. Intensive mechanical cleaning and strong disinfection wear a surface faster than traffic alone would suggest.
If the facility runs intensive cleaning or chemical disinfection — healthcare, food areas, laboratories — then treat abrasion and chemical resistance as a pair, and ask for both data sets.
Criterion 3 — Contamination and grit
Grit carried in from outside acts like abrasive paper underfoot, and entrance zones are where wear appears first.
If the floor is directly exposed to external grit and sand, then pair a higher wear group with entrance matting and a regime that removes grit before it spreads. If it is not, a mid-range group is usually the better economic choice.
Criterion 4 — Replacement cycle and lifecycle cost
A floor that must survive a long replacement cycle — hospitals, schools, transport buildings — carries a high cost of disruption when it is replaced early.
If the installation is permanent and disruption is expensive, then the higher wear group usually pays for itself. If the space is temporary or refurbished on a short cycle, then match the group to the expected life and put the saving where it shows.
Criterion 5 — Specification wording and verification
Write the requirement so that it can be checked: name the standard, require the report, and identify the product and thickness it must cover.
If a specification demands a group, then confirm which standard the requirement refers to (a wear group is not a use class), and ask for the abrasion test report for the exact product and thickness you are buying. If no report exists for that grade, request testing, select a construction that meets the criterion by design, or agree an equivalent specification in writing — never rely on a verbal claim.
Common Misreadings
| # | Common misreading | How to check it on the spot |
|---|---|---|
| 1 | Treating "Group T" as a universal specification | If the specification says only "Group T", with no standard number and no report requirement, the requirement is undefined — ask which standard and which report |
| 2 | Using a use class where a wear group is meant | Ask: "Is this the EN 660-2 group or the EN ISO 10874 use class?" Different standards, different dimensions |
| 3 | Treating a test classification as an approval | EN 660-2 is a method standard: describe the result as a classification, not an approval |
| 4 | Comparing groups across product types | Scope limits ranking to one product type — a group letter from another construction is not a like-for-like comparison |
| 5 | Accepting a report with a conclusion but no value | Look for the volume loss value, sample identification, laboratory and report number; if any is missing, the claim cannot be verified |
| 6 | Answering a slip question with a wear group | Wear is EN 660-2; slip is DIN EN 16165 (R classes); fire is a separate classification again |
| 7 | Using the wear group as the only selection criterion | Selection has four inputs: traffic intensity, wear group, substrate and installation quality, and the maintenance the facility will actually deliver |
| 8 | Presenting an in-house reading as a third-party conclusion | A report must trace to a named laboratory; an internal reading is a working reference, and should be described as one |
Table 4 — Common misreadings and how to check them.
FAQ
What is EN 660-2, and what do the F / M / P / T groups mean?
EN 660-2 is the European test method that measures how much material a PVC wear layer loses under the Frick-Taber abrasion test. Results are expressed as volume loss (Fv) and grouped into four classes — T (best), P, M and F.
Is wear group T the same as use class 33?
No — they are separate dimensions. EN 660-2 describes the abrasion resistance of the wear layer, while EN ISO 10874 classifies the intensity of traffic a floor is intended to handle, for example classes 31–34 for commercial areas. A product can be Group T and still be specified for lighter use, or the reverse.
How long will a Group T floor actually last?
A wear group is a laboratory ranking, not a service-life guarantee. In-service durability also depends on product construction, subfloor preparation, adhesive, installation quality, cleaning regime and the type of grit and traffic on site. Two floors in the same wear group can perform very differently under real conditions.
What should I check on an EN 660-2 abrasion report?
Check the testing laboratory and its accreditation, the standard and edition cited, sample identification (product, thickness, batch), the test conditions, the reported volume loss value, the resulting wear group, plus the report number and date. A wear group printed without a tested value or laboratory identification cannot be verified independently.
Does Group T mean the floor is slip-resistant?
No. Abrasion resistance and slip resistance are different properties, tested to different standards. Wear group comes from EN 660-2; slip resistance is measured under DIN EN 16165, which replaced DIN 51130, and is reported as R classes such as R9–R11. Always specify the two separately in a tender.
My specification demands Group T. What should I do?
Ask the supplier for the abrasion test report for the exact product and thickness you are buying, and confirm which laboratory issued it. If no report exists for that grade, request testing, select a construction that meets the criterion by design, or agree an equivalent specification in writing — never rely on a verbal claim.
Wear Class Is a Specification Decision, Not a Marketing Claim
Wear group selection rewards the buyer who asks for the value, the sample reference and the laboratory — and who writes the requirement so that someone else can check it. That is what EN 660-2 is for: comparing wear layers on measured evidence inside a product type, rather than on adjectives.
We publish the criteria, explain how to read the report, and provide test documentation on request — so you can verify the grade instead of trusting it.
Next step: tell us the application, the traffic level the area is designed for, and the group your specification requires. We will confirm which construction fits, state the standard and value each claim rests on, and send the abrasion test report for the exact product and thickness on request.
Contact our technical team · See how to read a flooring test report
Further reading on this site:
- Flooring standards guide: which test report to request and how to read it
- How to read a flooring test report
- Flooring glossary: wear layer, use class, slip resistance
- Homogeneous vinyl flooring for high-traffic areas
- Hospital flooring: homogeneous vinyl vs SPC
Standards referenced: EN 660-2:1999 (Resilient floor coverings — Determination of wear resistance — Part 2: Frick-Taber test, BSI record · CEN/iTeh record); EN ISO 10874 (classification of resilient floor coverings by use); DIN EN 16165:2021-12 (determination of slip resistance, formerly DIN 51130); EN ISO 10581, EN ISO 10582, EN ISO 11638 (product specification standards for resilient sheet flooring).